    ASTM D3359 is a tape test to check adhesion of the coating for its intended use before the part ships. In ASTM D3359 adhesion test, cuts are made through the coating to the substrate. Then pressure-sensitive tape is applied over the cut and pulled off. The amount of coating removed is rated.

    The ASTM D3359 standard has two methods: the X-Cut Test and Cross-Cut Test. X-Cut Test is primarily intended for thicker coatings and the Cross-Cut Test is primarily intended for thinner ones. Manufacturers, applicators and quality teams in aerospace, automotive, energy and other industries use ASTM D3359 for quality control, process verification, coating comparison and failure investigation.

    Infinita Lab delivers ASTM D3359 coating adhesion tape testing through accredited U.S. partner labs. You receive an independent report with the adhesion rating, the test performed and observations of coating removal. 

    What Is ASTM D3359?

     

    ASTM D3359 standard is a process to check the adhesion of coating films on metal substrates. It is done by making a cut on the film and then applying and removing pressure sensitive tape over it.

    Painted metal components, powder-coated parts, and metal surfaces with protective, anti-corrosion, decorative or industrial coatings are the material tested with ASTM D3359. These applications are found across aerospace, automotive, energy, chemical, electrical and electronics, consumer goods, medical device and packaging industries.

    ASTM D3359 includes two testing methods: the X-Cut Test (Method A) and the Cross-Cut (Cross-Hatch) Test (Method B). In both tests, cuts are made through the coating to the substrate and then pressure-sensitive tape is applied over the cuts and removed. The coating condition is rated on a scale from 0 to 5 with the letter A or B to show which test method was performed. The test method is chosen based on coating thickness.

    What Is the ASTM D3359 X-Cut Test?

     

    The X-Cut Test is a method to evaluate thicker coating adhesion by making two cuts intersecting each other to create an “X” through the coating film to the substrate. Then pressure-sensitive tape is applied over the intersection and removed.

    When Does the X-Cut Test Apply?

    The ASTM D3359 Method A applies when:

    • Coating: greater than 5 mils (125 µm) thick
    • Testing is performed in the field or on installed parts and structures (it can also be done in the shop or laboratory)
    • The coating is a relatively ductile film on a metallic substrate

    What Is the ASTM D3359 Cross-Cut (Cross-Hatch) Test?

     

    The Cross-Cut Test, also called the Cross-Hatch Test, is a method that cuts a lattice pattern through the thinner coating to the substrate. Then pressure-sensitive tape is applied over the grid and removed.

    When Does the Cross-Cut (Cross-Hatch) Test Apply?

     

    The ASTM D3359 Method B Test applies when:

    • Coating: less than 5 mils (125 µm) thick
    • Testing is performed in a laboratory or shop (it can also be done in the field)
    • The coating is a relatively ductile film on a metallic substrate

    How Many Cuts Are Required for the Cross-Hatch Test?

     

    The number of cuts and their spacing depend on coating thickness:

    Coating thicknessCuts in each directionCut spacing
    Up to 2 mils (50 µm)111 mm
    2 to 5 mils (50–125 µm)62 mm

    What Is the Difference Between the X-Cut Test and the Cross-Cut (Cross-Hatch) Test?

    The main difference between the X-Cut Test and the Cross-Cut (Cross-Hatch) Test is the cut pattern which is selected by coating thickness. The X-Cut Test uses a single “X” and is intended for coatings thicker than 5 mils. On the other hand, the Cross-Cut Test uses a lattice and is intended for coatings thinner than 5 mils.

     


    Basis
    X-Cut TestCross-Cut (Cross-Hatch) Test
    Cut patternSingle “X”Lattice of 6 or 11 cuts per direction
    Coating thicknessGreater than 5 mils (125 µm)Less than 5 mils (125 µm)
    Primarily intended forField testingLaboratory and shop testing
    Cut spacingNot applicable1 mm or 2 mm, based on thickness
    Rating scale0A to 5A0B to 5B

    ASTM D3359 Scope, Applications and Benefits for Coating Adhesion Testing

    Scope

    Scope of ASTM D3359

    • Test method selected by thickness: The X-Cut Test is intended for coatings thicker than 5 mils (125 µm). The Cross-Cut (Cross-Hatch) Test is intended for those thinner than 5 mils (125 µm).
    • Thickness must be known: If the total coating thickness has not been determined, it should be measured first using a standard such as ASTM D7091 or another method agreed on by the interested parties.
    • Checks adhesion is good enough: The test determines if the coating is bonded good enough for its intended use. It cannot tell how strong the adhesion is. 
    • Primarily for metal surfaces: ASTM D3359 was developed for coatings on metal surfaces. It has been used on materials such as wood and plastic but there is no precision and bias data to show how reliable the results are on those materials.
    • Layered coatings can fail between layers: In case of several layers, the tape may pull off one layer from another instead of pulling the coating off the metal. If that happens, the test does not show how well the whole coating system is bonded to the substrate.

    Applications

    Applications of ASTM D3359 Coating Adhesion Testing

      • Quality control of finished coatings: checking that painted, primed, or coated parts meet adhesion requirements before shipment. This helps catch adhesion problems before they reach the customer.
      • Surface preparation and process verification: evaluating the effect of cleaning, pretreatment, application, and curing on adhesion. Surface preparation has a strong influence on how well a coating bonds, so the test shows whether the process is working.
      • Comparing coatings, substrates, and surface treatments: ranking different coatings on the same substrate, or the same coating on different substrates or treatments. This supports material and process selection.
      • Evaluating adhesion after environmental exposure: assessing coatings after salt spray, UV exposure, accelerated aging, or fluid immersion. Comparing results before and after exposure shows how well the bond holds up.
      • Failure investigation: diagnosing peeling, flaking, and delamination in coated parts and structures. Testing affected and unaffected areas can help narrow down the cause.
      • Coating development and R&D: screening new formulations and application methods. Quick results let development teams compare candidates early.
      • Field inspection and maintenance: checking the condition of coatings already in service on installed equipment and structures. The X-Cut Test is commonly used for this kind of on-site work.
      • Specification and OEM compliance: documenting that a coating meets the adhesion requirement in a customer or industry specification. The specification sets the acceptable rating, and the test provides the evidence.

    Benefits

    Benefits of ASTM D3359 Tape Testing

      • Fast and simple: the test takes very less time and does not require complex setup or instrumentation. Results are available as soon as the tape is removed and the area is inspected.
      • Low cost: minimal equipment makes it practical for routine and high-volume checks. Teams can test more samples without a large investment.
      • Flexible testing locations: it can be performed in the laboratory, in the shop, or in the field. The X-Cut Test is commonly used on-site and the Cross-Cut Test is commonly used in the laboratory.
      • Standardized, comparable results: a defined procedure and rating scale let results be compared across samples and batches when the test is performed consistently. A common method also reduces disagreement about how adhesion was judged.
      • Early detection of problems: it flags adhesion weaknesses before coated parts reach service. Finding a problem at this stage is typically less costly than a failure in the field.
      • Process feedback: the visible result helps teams trace adhesion problems back to surface preparation, application, or curing. This points corrective action to the right step.
      • Support for specifications: it provides documented evidence for customer, OEM, and quality-system requirements. A recorded rating gives a clear basis for acceptance decisions.

    Our ASTM D3359 Testing Procedure

    Surface Preparation

    The coated test area is cleaned of dirt, oil and loose debris.It should be free of blemishes and surface imperfections. The coating is conditioned as the specification requires, because extremes of temperature or humidity can affect the results.

    1

    Cut Pattern Formation

    Using a sharp blade and a straightedge or cutting guide, the technician cuts through the coating to the substrate in one steady motion. The X-Cut Test uses two intersecting cuts at an angle of 30° to 45°. The Cross-Cut (Cross-Hatch) Test uses a lattice of 6 or 11 cuts in each direction, spaced to match the coating thickness.

    2

    Tape Application

    In ASTM D3359 tape test, Pressure-sensitive tape is centered over the cuts and smoothed into place by finger. It is then rubbed firmly with a pencil eraser to ensure full contact with the coating. The tape type is one agreed on by the parties involved, since a single tape may not suit every coating.

    3

    Tape Removal & Evaluation

    Within 90 ± 30 seconds of application, the tape is pulled off rapidly at an angle as close to 180° as possible. The test area is then inspected under good lighting and rated from 0 to 5 with the letter A for the X-Cut Test or B for the Cross-Cut Test.

    4

    ASTM D3359 Test Parameters and Requirements

    ParameterDetails
    StandardASTM D3359, Standard Test Methods for Rating Adhesion by Tape Test
    TestsX-Cut Test and Cross-Cut (Cross-Hatch) Test
    SubstrateMetallic substrates (developed with metal as the substrate)
    Coating typeRelatively ductile coating films
    Coating thickness: X-Cut TestPrimarily intended for coatings and coating systems greater than 5 mils (125 µm)
    Coating thickness: Cross-Cut TestPrimarily intended for coatings and coating systems less than 5 mils (125 µm). It may be used on thicker films with wider-spaced cuts when the purchaser and seller explicitly agree.
    Thickness measurementRequired if the thickness is not already known, using a standard such as ASTM D7091 or another method agreed on by the interested parties
    Cut pattern: X-Cut TestTwo intersecting cuts through the coating to the substrate, with a smaller angle of 30° to 45°
    Cut pattern: Cross-Cut TestLattice of 6 or 11 cuts in each direction through the coating to the substrate
    Cut spacing: Cross-Cut Test1 mm for coatings up to 2 mils (50 µm), 2 mm for coatings from 2 to 5 mils (50–125 µm)
    Cutting guideSteel or other hard metal straightedge or template for straight cuts
    TapePressure-sensitive tape, 1 inch (25 mm) wide and semitransparent, with an adhesion strength agreed on by the interested parties
    Tape applicationCentered over the cuts, smoothed by finger, then rubbed firmly with a pencil eraser
    Tape removalWithin 90 ± 30 seconds of application, pulled off rapidly, not jerked, at an angle as close to 180° as possible
    Test environmentExtremes of temperature or relative humidity can affect the tape or the coating
    Rating scale0A to 5A (X-Cut Test) and 0B to 5B (Cross-Cut Test), reported as whole numbers only, with 5 as the best result
    Result typeQualitative adhesion rating, not a measured bond strength
    Rating scale0A to 5A (X-Cut Test) and 0B to 5B (Cross-Cut Test), reported as whole numbers only, with 5 as the best result
    Result typeQualitative adhesion rating, not a measured bond strength
    Acceptance criteriaSet by the coating specification, customer, or OEM, not by the standard
    Operator requirementTrained and practiced operators, because the angle and rate of tape removal and the visual assessment affect results
    • Cross-hatch cutter or sharp blade
    • Pressure-sensitive adhesive tape
    • Magnifying lens or microscope
    • Cleaning materials
    • Inspection tools

    Equipment and Instrumentation Used for ASTM D3359 Testing

    What You Receive: ASTM D3359 Test Report and Results

    • Adhesion rating (0B to 5B)
    • Test method used (A or B)
    • Observations of coating removal
    • Sample identification details
    • Compliance statement with ASTM D3359

    ASTM D3359 Coating Adhesion Tape Test FAQs

    Yes. Extremes of temperature or relative humidity can affect the adhesion of the tape or the coating. Testing should follow any conditions set in the coating specification.

    Yes. The cuts go through the coating to the substrate, so the tested area is damaged. Testing is usually done on test panels or in locations where the damage is acceptable and the specification may call for repair.

    No. ASTM D3359 is a qualitative test that indicates adhesion is adequate or not for the application. It does not give the force needed to break the bond and it cannot distinguish between higher levels of adhesion.

    Only under specific conditions. The Cross-Cut Test is not considered suitable for films thicker than 5 mils unless wider-spaced cuts are used and the purchaser and seller explicitly agree.

    Each rating is a number from 0 to 5, where 5 is the best result. The letter shows which test was performed: A for the X-Cut Test and B for the Cross-Cut Test. The two scales are separate, so a 4A and a 4B should not be compared directly.

    Several factors can change the result: Tape: A given tape may not adhere equally well to different coatings, so no single tape suits every coating. Environment: Extremes of temperature or relative humidity can affect the tape or the coating.

    Yes. The test is commonly used to check how well a coating stays bonded after exposure such as salt spray, UV, accelerated aging, or fluid immersion. The specification typically defines the exposure conditions and the required rating.

    Why Choose Infinita Lab for Coating Adhesion Tape Testing

    When your Coating Adhesion Tape results have to hold up - for compliance, a customer audit, or an engineering decision - ASTM D3359 accuracy and an unbiased third-party report matter more than price. Infinita Lab routes your ASTM D3359 coating adhesion tape testing to ISO/IEC 17025-accredited U.S. partner labs with hands-on method experience, so you get defensible data, transparent reporting, and turnaround times built around your project deadline - not ours.

    brain

    Need ASTM D3359 Coating Adhesion Tape Testing You Can Rely On?

    Send query us at hello@infinitalab.com or call us at (888) 878-3090 to learn more about our services and how we can support you.

     Request a Quote

    Request a Quote

    Submit your material details and receive testing procedures, pricing, and turnaround time within 24 hours.



    • ddd
      Quick Turnaround and Hasslefree process
    • ddd
      Confidentiality Guarantee
    • ddd
      Free, No-obligation Consultation
    • ddd
      100% Customer Satisfaction
    Home / Services / ASTM D3359: Coating Adhesion Tape Testing Services
    ×

    Talk to an Expert

      Connect Instantly

      (888) 878-3090
      Ensure Quality with the Widest Network of Accredited Labs
      • ddd
        Quick Turnaround and Hasslefree process
      • ddd
        Confidentiality Guarantee
      • ddd
        Free, No-obligation Consultation
      • ddd
        100% Customer Satisfaction

        ddd

        Start Material Testing